Screen printing is the workhorse metallization step in solar cell manufacturing, but the mechanical pressure and thermal treatment involved can harm the sensitive passivating contact stacks of heterojunction devices. The problem is especially relevant for copper-plated silicon heterojunction (SHJ) cells, which are pursued as a way to cut metallization costs and reduce dependence on silver, yet whose amorphous silicon/crystalline silicon interfaces are easily degraded by added recombination.
Researchers in China have now examined how the printing step causes that damage and proposed a modified screen design intended to limit it. The work was published in the journal Solar Energy.
A different contact regime from silver paste
Corresponding author Lang Zhou explained that photoresist printing in SHJ production differs fundamentally from conventional silver paste printing. In silver paste screens, the openings account for only 2–5% of the total area, and an emulsion layer covers the remainder, preventing the mesh from touching the wafer. Full-area photoresist coating, by contrast, typically uses a screen without emulsion coverage so that the resist is deposited evenly across the whole wafer, which means the mesh comes into direct and extensive contact with the wafer during every printing cycle.
Production data cited by the team had already shown conversion efficiency declining from 26.2% to 25.7% over 15,000 consecutive printing cycles. The losses were concentrated in open-circuit voltage and fill factor, while short-circuit current density and electrical resistance remained largely unchanged. Minority carrier lifetime degradation rose from 0.61% with a new screen to 11.0% after 15,000 cycles.
Worn knuckles, hidden damage
Using three-dimensional confocal microscopy, the scientists linked the decline to progressive wear of the screen mesh knuckles. As these knuckles flatten, their contact area with the wafer grows, increasing the mechanical stress transferred to the underlying passivation layers. Scanning electron microscopy revealed no visible surface scratches, but photoluminescence measurements confirmed higher recombination losses, pointing to damage at the amorphous/crystalline silicon interface.
To interrupt the direct contact, the researchers added an emulsion buffer layer to the screen and evaluated six patterns with emulsion coverage ratios between 2.9% and 16.6%. The trials exposed a trade-off: greater emulsion coverage reduced mechanical damage but impaired photoresist distribution. A coverage ratio of 4.7% provided the best balance, holding minority carrier lifetime degradation to 0.41% after 10,000 printing cycles while maintaining relatively good coating uniformity.
The team attributed the improvement to the emulsion layer keeping the mesh away from the wafer surface, thereby limiting cumulative mechanical damage to the sensitive passivation layers. Zhou said the findings show that a relatively simple modification to screen design can substantially mitigate printing-induced degradation, offering a practical approach to improving manufacturing reliability for copper-plated SHJ cells.
Copper metallization gains momentum
The results arrive as copper attracts growing interest as a substitute for silver contacts. In April 2026, researchers at China's Nankai University reported a silver-free SHJ cell with 25.2% efficiency, using plasma-induced interface engineering and copper electroplating to address adhesion, contact resistance and stability challenges at the ITO interface. Separately, scientists at Germany's Forschungszentrum Jülich achieved 23.08% efficiency in a fully copper-metallized SHJ cell, a relatively small penalty compared with its silver-metallized counterpart, while a hybrid design combining silver-copper paste on the front with silver contacts on the rear reached 23.95%. Those results underline copper's potential to reduce silver consumption, although further work on processing and electrical performance is still needed.